6.6.3 Lining Defects and Their Causes

Inspection, assessment, repair and clearance improvement of existing railroad tunnels and their portals.
Author: Daniel P. Colwell
6.6.3 Lining Defects and Their Causes

The pattern of a defect usually shows its cause. Interpreting the pattern correctly decides whether a repair is cosmetic or structural.

Table 6.6-2. Lining defects, likely causes and significance
DefectLikely causeSignificance
Longitudinal crack along the crownVertical ground load greater than the lining was built for; loss of support at the springlines; voids above the crown letting the arch deformStructural. Check for flattening of the crown and for voids above it. Monitor crack width.
Longitudinal cracks at the springlines or walls, with bulgingLateral ground pressure, often from swelling or squeezing ground or from water pressure behind the liningStructural. Measure the profile and monitor convergence.
Transverse cracks at regular spacingShrinkage and temperature change in plain concrete placed in long poursUsually not structural, but a path for water and ice.
Diagonal cracks near portalsMovement of the slope or portal structure; differential settlementStructural. Check portal slope stability (Section 6.6.6).
Spalling and delaminationFreeze-thaw near portals; corrosion of reinforcement; locomotive exhaust and moisture; impactFalling concrete is a hazard to trains and workers. Sound and remove loose material.
Lost mortar, open joints, dropped bricks or stonesWater flowing through joints; freeze-thaw; ageLoss of arch action if extensive. Repoint, and fix the water source.
Ring separation in brick archesWeathering of the mortar between rings; cyclic loadingReduces arch capacity. Investigate by coring or GPR.
Leakage and mineral depositsWater passing through cracks, joints and cold jointsIce at the portals, corrosion, fouled ballast, and washing of fines from behind the lining.
Floor heave and track profile changesSwelling or squeezing rock in the invert; frost; poor drainageTrack geometry defects. See Section 6.6.5.

Voids behind old linings deserve particular attention. Where concrete was placed against timber lagging or against overbreak without backfill, the timber rots and the voids remain. A rock block can then fall onto the lining from above as a point load, which a plain concrete arch cannot carry. GPR along the crown, followed by drilling, finds these voids; contact grouting fills them.

For railroad work: A new or widening longitudinal crack in the crown, a flattening of the arch, or fresh spalling over the track calls for a prompt in-depth inspection and, until it is done, a slow order or a protective measure (temporary support or netting). Photograph and measure cracks each time so that change, not just presence, is recorded.