2.12.2 Sulfate Heave in Stabilized Subgrades

Ground chemistry that attacks concrete, heaves stabilized subgrades and turns fresh shale into soil within a few seasons of exposure.
Author: Daniel P. Colwell
2.12.2 Sulfate Heave in Stabilized Subgrades

When lime or cement is mixed into a sulfate-bearing clay, calcium, aluminum (from the clay) and sulfate combine in the presence of water to form ettringite, a mineral that occupies a much larger volume than its ingredients. The result is heave of a stabilized subgrade weeks to months after construction, often in a pattern of humps that is hard to repair. The risk depends on the soluble sulfate content of the soil.

Table 2.12-2. Sulfate content and calcium-based stabilization (typical agency guidance; varies by state)
Soluble sulfate (ppm)RiskTypical response
< 3,000LowOrdinary lime or cement stabilization
3,000 to 5,000ModerateExtended mellowing (24 to 72 hr) after lime and water; extra water; or alternative stabilizer
5,000 to 8,000Moderate to highDouble application with mellowing, or non-calcium stabilizer; project-specific testing
> 8,000HighAvoid calcium-based stabilization; remove and replace or use mechanical stabilization

Sulfate in clay is often patchy, concentrated in gypsum crystals and seams. Sample at close spacing along the alignment and test the soluble sulfate (for example, TxDOT Tex-145-E or AASHTO T 290). Water used in construction can also bring sulfate in; test it too. Stabilization methods are described in Chapter 7.2 and Chapter 7.3.