Water-soluble sulfates (mainly from gypsum and sodium and magnesium sulfates) react with the hydrated cement in concrete to form expansive products that crack and soften it. Culverts, footings, piles, retaining walls and drainage structures in contact with sulfate-bearing soil or water are at risk. Design is by exposure class, based on the water-soluble sulfate content of the soil or the sulfate concentration in the water.
| Class | Water-soluble SO4 in soil (% by mass) | SO4 in water (ppm) | Typical requirements |
|---|---|---|---|
| S0 | < 0.10 | < 150 | No special requirement |
| S1 | 0.10 to < 0.20 | 150 to < 1,500 | Moderate sulfate resistance (e.g., Type II); w/cm ≤ 0.50; f′c ≥ 4,000 psi |
| S2 | 0.20 to 2.00 | 1,500 to 10,000 | High sulfate resistance (e.g., Type V); w/cm ≤ 0.45; f′c ≥ 4,500 psi |
| S3 | > 2.00 | > 10,000 | Type V plus pozzolan or slag; w/cm ≤ 0.45; f′c ≥ 4,500 psi |
Note the units: laboratories often report soil sulfate in parts per million (mg/kg). 1,000 ppm equals 0.10% by mass. Precast culvert and pipe suppliers should be given the exposure class in the specifications.