↑ Parent Menu⌂ Main Menu
← Railway Ground Hazard Risk Management
GHRM
Railway Ground Hazard Risk Management · 2.0 · The Underworld
Sections · open a dropdown to go to a section or subsection

Chapter 2.12 — Sulfates, Sulfides and Problem Mudrocks

Ground chemistry that attacks concrete, heaves stabilized subgrades and turns fresh shale into soil within a few seasons of exposure.
Author: Daniel P. Colwell

Some ground problems are chemical rather than mechanical. Sulfate in soil and groundwater attacks concrete and reacts with lime and cement to form expansive minerals. Pyrite (iron sulfide) in shale oxidizes when exposed to air and water, producing acid and sulfate and swelling the rock. Many shales and claystones slake and lose strength within months of excavation. This chapter covers how to recognize these conditions, the tests that identify them and the design responses for concrete, stabilization and cut slopes.

Further reading — ICE Manual of Geotechnical Engineering
The chapters below cover the same ground in more depth. They are cited, not reproduced; see Appendix G for the full cross-reference and edition notes.
2.12.0 Purpose and Overview

These problems share two features. First, they are invisible in an ordinary boring log: a gray clay with sulfate or a dark shale with pyrite looks the same as one without. Second, they are triggered by the project itself: by adding lime or cement, by placing concrete, or by exposing rock to air and water in a cut. The investigation has to test for them specifically, and the trigger is something the designer controls.

2.12.1 Sulfate Attack on Concrete

Water-soluble sulfates (mainly from gypsum and sodium and magnesium sulfates) react with the hydrated cement in concrete to form expansive products that crack and soften it. Culverts, footings, piles, retaining walls and drainage structures in contact with sulfate-bearing soil or water are at risk. Design is by exposure class, based on the water-soluble sulfate content of the soil or the sulfate concentration in the water.

Table 2.12-1. Sulfate exposure classes (after ACI 318; check the edition in force for the project)
ClassWater-soluble SO4 in soil (% by mass)SO4 in water (ppm)Typical requirements
S0< 0.10< 150No special requirement
S10.10 to < 0.20150 to < 1,500Moderate sulfate resistance (e.g., Type II); w/cm ≤ 0.50; f′c ≥ 4,000 psi
S20.20 to 2.001,500 to 10,000High sulfate resistance (e.g., Type V); w/cm ≤ 0.45; f′c ≥ 4,500 psi
S3> 2.00> 10,000Type V plus pozzolan or slag; w/cm ≤ 0.45; f′c ≥ 4,500 psi

Note the units: laboratories often report soil sulfate in parts per million (mg/kg). 1,000 ppm equals 0.10% by mass. Precast culvert and pipe suppliers should be given the exposure class in the specifications.

2.12.2 Sulfate Heave in Stabilized Subgrades

When lime or cement is mixed into a sulfate-bearing clay, calcium, aluminum (from the clay) and sulfate combine in the presence of water to form ettringite, a mineral that occupies a much larger volume than its ingredients. The result is heave of a stabilized subgrade weeks to months after construction, often in a pattern of humps that is hard to repair. The risk depends on the soluble sulfate content of the soil.

Table 2.12-2. Sulfate content and calcium-based stabilization (typical agency guidance; varies by state)
Soluble sulfate (ppm)RiskTypical response
< 3,000LowOrdinary lime or cement stabilization
3,000 to 5,000ModerateExtended mellowing (24 to 72 hr) after lime and water; extra water; or alternative stabilizer
5,000 to 8,000Moderate to highDouble application with mellowing, or non-calcium stabilizer; project-specific testing
> 8,000HighAvoid calcium-based stabilization; remove and replace or use mechanical stabilization

Sulfate in clay is often patchy, concentrated in gypsum crystals and seams. Sample at close spacing along the alignment and test the soluble sulfate (for example, TxDOT Tex-145-E or AASHTO T 290). Water used in construction can also bring sulfate in; test it too. Stabilization methods are described in Chapter 7.2 and Chapter 7.3.

2.12.3 Pyrite and Sulfide Oxidation

Pyrite (FeS2) is common in dark shales, coal measures and some slates and organic clays. While it stays buried below the water table it is stable. When a cut or excavation exposes it to air and water it oxidizes, producing sulfuric acid, iron hydroxide staining and sulfate. The consequences are:

  • Heave: sulfate reacts with calcite in the rock to form gypsum, which occupies about twice the volume. Floor slabs, footings and backfill on pyritic shale or pyritic shale fill have heaved several inches over a few years.
  • Acid drainage: low-pH water with dissolved iron and metals from cut slopes and spoil, staining ditches orange and attacking concrete and steel.
  • Secondary sulfate attack on concrete from the sulfate produced.
  • Faster degradation of the rock itself as acid and crystal growth open fractures.

Screening tests include total sulfur, pyritic sulfur, acid-base accounting (acid-producing potential vs. neutralizing potential) and paste pH. Do not use pyritic shale as structural fill under slabs or behind walls, and do not let pyritic spoil drain to streams without treatment.

2.12.4 Slaking and Degradable Mudrocks

Many shales, mudstones and claystones are rock in the boring and soil a few seasons after the cut is opened. Wetting and drying, unloading and frost break them down along bedding, and the debris accumulates in ditches, fouls ballast and falls on the track. Durability is measured by the slake durability index (ASTM D4644, withdrawn 2025), with the second-cycle value Id2 usually reported.

Table 2.12-3. Slake durability classification (second cycle)
Id2 (%)DurabilityBehavior in cuts and fills
0 to 30Very lowDegrades to soil within months; treat as soil for slopes and fill
31 to 60LowSlakes in a few seasons; flatten cuts or protect faces
61 to 85MediumGradual surface degradation; ditch cleaning
86 to 95HighDurable with normal design
96 to 100Very highDurable

Low-durability mudrocks placed as rockfill break down after placement and cause settlement of the embankment, so they should be compacted in thin lifts as soil. In cuts, design benches and ditches to catch debris, and consider shotcrete or vegetation for faces in very low durability rock. Rock slope stability is covered in Chapter 2.7.

2.12.5 Testing Program
Table 2.12-4. Tests for chemically problematic ground
ConcernTestSample
Sulfate attack on concreteWater-soluble sulfate (soil); sulfate (water); pH; chlorideSoil at foundation and culvert levels; groundwater
Sulfate heave with lime or cementSoluble sulfate at close spacing; trial mix swell testSubgrade to depth of stabilization
Pyrite oxidationTotal and pyritic sulfur; acid-base accounting; paste pHDark shales, coal measures, organic clays
Mudrock durabilitySlake durability (ASTM D4644, withdrawn 2025); jar slake testFresh core from the cut
Corrosion of steelResistivity, pH, chloride, sulfateSoil and water at pile and anchor depths

These tests are inexpensive and are best added to the laboratory program from the start (Chapter 5.2), since resampling after a problem appears is costly.

2.12.6 Worked Example
The example uses a generic site and is not taken from any client project. It follows the five-part format.
Example 2.12-1: Concrete Exposure Class and Stabilization Decision for a Sulfate-Bearing Clay

A new box culvert and a lime-stabilized subgrade are planned in a gray clay with visible gypsum crystals. The laboratory reports water-soluble sulfate of 4,200 ppm in the clay at culvert level and 3,600 ppm in the subgrade samples.

Given

VariableValueDescription
SO4 (culvert)4,200 ppmWater-soluble sulfate in clay at culvert level
SO4 (subgrade)3,600 ppmHighest value in the stabilization zone
Conversion1% = 10,000 ppmPercent by mass to ppm
Exposure limitsTable 2.12-1Sulfate exposure classes
Lime limitsTable 2.12-2Sulfate heave risk bands

Required

  • Sulfate exposure class and concrete requirements for the culvert
  • Whether ordinary lime stabilization is suitable

Equations

  1. Eq. 1: % by mass = ppm / 10,000 — unit conversion

Steps

Step 1 · Convert culvert value
4,200 / 10,000 = 0.42% by mass
0.42%
Spot check: Between 0.20 and 2.00% by mass.
↓
Step 2 · Exposure class
0.20 ≤ 0.42 ≤ 2.00 (Table 2.12-1)
Class S2
Spot check: S1 tops out at 0.20% (2,000 ppm); 4,200 ppm is above that.
↓
Step 3 · Stabilization risk
3,600 ppm is in the 3,000 to 5,000 band (Table 2.12-2)
Moderate risk
Spot check: Below 5,000 ppm, so not in the high band, but above the 3,000 ppm low-risk limit.
↓
Solution
The culvert is in exposure class S2 (high sulfate resistance, w/cm ≤ 0.45, f′c ≥ 4,500 psi). The subgrade is at moderate sulfate heave risk: ordinary lime stabilization is not suitable without extended mellowing or an alternative.

Solution

The culvert is in exposure class S2 (high sulfate resistance, w/cm ≤ 0.45, f′c ≥ 4,500 psi). The subgrade is at moderate sulfate heave risk: ordinary lime stabilization is not suitable without extended mellowing or an alternative.

The culvert specification should name class S2 so that the precast supplier uses sulfate-resisting cement and the required water-cement ratio. Backfill around the culvert should not be lime- or cement-treated clay from the same deposit.

For the subgrade, the options are a lime application with 48 to 72 hours of mellowing at extra moisture before compaction, supported by a laboratory swell test on the actual soil, or a mechanical stabilization (geogrid and granular section) that avoids calcium altogether. Because sulfate in gypsiferous clay is patchy, more samples along the alignment are needed before choosing: a single 8,000 ppm pocket would rule out lime.

2.12.7 Cross-References

Related chapters in this manual:

Related ICE Manual chapters are listed in the Further Reading box at the top of this chapter and in Appendix G.

← Previous · 2.0 The Underworld Chapter 2.11 — Soluble Ground and Karst: Sinkholes, Voids and Dissolution
Next · 2.0 The Underworld → Chapter 2.13 — Residual, Tropical and Arid Soils