7.4.8 Concrete Culverts, Walls and Abutments: Deterioration, Assessment and Repair

Treating the cuts and embankments of a railroad as an asset portfolio: inventory, condition, deterioration, prioritization and the choice of remedial works.
Author: Daniel P. Colwell
7.4.8 Concrete Culverts, Walls and Abutments: Deterioration, Assessment and Repair

The earthworks inventory (Section 7.4.1) includes concrete and masonry structures that hold the earthworks together: culverts and their headwalls, retaining walls, wing walls, abutments and the footings of piers and signal structures. Their failure is a ground hazard even when the cause is the concrete, because a collapsed culvert or a failed wall takes the embankment with it. This section covers how concrete in these structures deteriorates, how to assess it, and the repair choices, drawing on the proceedings of the 2nd International Conference on Concrete Repair, Rehabilitation and Retrofitting (Cape Town, 2008).

The economics are summarized by de Sitter’s “rule of fives”, quoted by Walraven (2009): if maintenance is skipped, the later repair costs about five times the maintenance saved; if repair is skipped, renewal costs about five times the repair saved. Early condition assessment and timely repair are therefore part of the risk reduction in Chapter 3.8, not an optional extra.

7.4.8.1 How concrete deteriorates

  • Chloride-induced corrosion of reinforcement, from deicing salt at grade crossings and on overhead structures, salt-laden runoff, and sea water. It is the most common cause of serious damage, together with carbonation.
  • Carbonation of the cover concrete, which lowers the pH around the steel until it can corrode. It is slow in good, wet concrete and fast in porous, partly dry concrete with thin cover.
  • Freeze–thaw damage, worse with deicing salts and in saturated concrete such as culvert inverts, headwalls and wall faces that stay wet.
  • Chemical attack: sulfate attack from sulfate-bearing soil and groundwater (Chapter 2.12), and acid attack. Culverts that carry sewage-affected flow can suffer biogenic sulfuric acid attack above the water line, as in concrete sewers.
  • Alkali-aggregate reaction (AAR): the reaction of alkalis in the cement with reactive silica in the aggregate forms a gel that swells and causes map cracking and longitudinal cracks, often years after construction.

Critical chloride content. Angst and Vennesland (2009) reviewed about 40 studies of the chloride content at which steel starts to corrode. Reported values ranged from 0.02% to 3.08% chloride by weight of cement, so no single threshold exists; the steel–concrete interface, the pH of the pore water and the electrochemical potential of the steel all control it. In practice, owners set decision levels: on one set of marine bridges, members with more than 1% chloride by weight of cement at the steel were judged too contaminated for coatings and inhibitors and were either treated electrochemically or rebuilt (Streicher et al. 2009).

7.4.8.2 Condition assessment and nondestructive testing

  • Visual mapping of cracks, spalls, rust stains, efflorescence, scaling, exposed steel and wall movement, tied to stations and photographs (Section 7.4.2).
  • Cores for strength, chloride profiles and carbonation depth, and petrography for AAR. Fischboeck and Harmuth (2009) combined visual examination, a damage rating index from polished sections, ultrasonic pulse velocity and resonant frequency to identify and rank AAR damage; profiles of dynamic modulus from pulse velocity located the worst-damaged zones.
  • Ultrasonic pulse-echo with low-frequency, dry point-contact transducers and synthetic-aperture imaging measures thickness and finds voids, delaminations and ungrouted ducts from one face (Wiggenhauser 2009). Ground-penetrating radar locates reinforcement and measures cover, and electrical resistance tomography maps reinforcement and moisture.
  • Culverts: a CCTV survey alone does not give a complete assessment. Da Silva and Goyns (2009) calibrated CCTV with physical measurements, including windows cut through the pipe wall to measure the actual loss of material, and assessed the pipe and surrounding soil as one system. Leaks out of a culvert carry soil with them and create voids under the track (Chapter 2.1, Section 2.1.5; Chapter 2.11).
  • Reliability of NDT. Methods should be validated against reference specimens or cores before they are relied on for decisions, and combining methods gives more reliable results than any one alone.

7.4.8.3 Repair and protection options

Table 7.4-8. Repair and protection options for reinforced concrete earthwork structures
OptionWhat it doesNotes for use
Water repellent (silane) impregnationKeeps water and chlorides out of sound concreteWorks only if it penetrates deeply enough. Johansson et al. (2009) found that extending contact time from 1 to 5 hours (for example by using a paste or gel rather than a liquid) about doubles the depth, as do drier concrete and higher porosity. Check depth by splitting a treated core and wetting it.
Corrosion inhibitorsSlow corrosion of steel in contaminated concreteLess effective at high chloride levels.
Patch repairReplaces damaged concrete around the steelBond depends more on an undamaged substrate than on roughness. Bissonnette et al. (2009) found that jackhammering leaves a damaged surface that outweighs its extra roughness; hydrodemolition, scarifying and blasting gave better bond. Verify with pull-off tests.
Galvanic (sacrificial) anodesZinc anodes connected to the steel corrode instead of itNo power supply; typical design life about 25 years. Anode mortar dosages of roughly 0.1 lb per ft² of steel surface have been used (Bänziger et al. 2009). Can be checked during routine inspections by measuring anode current.
Impressed-current cathodic protectionA power supply drives protective current to the steelLong-lived; needs monitoring and maintenance of the power supply.
Electrochemical chloride extractionA temporary external anode draws chlorides out of the cover and raises the pH at the steelTreatment over weeks; seal the surface afterward to stop new chlorides. Treated bridge members showed no new spalling or rust staining after four years (Streicher et al. 2009).
Realkalisation and hybrid treatmentsRestore high pH at the steelA brief impressed-current “pit realkalisation” of 1 to 2 weeks, followed by galvanic protection from the same installed anodes, arrests and then prevents corrosion (Glass et al. 2009).
Externally bonded FRPRestores or adds flexural and shear strengthFor walls, caps and beams; needs sound substrate and anchorage at the ends.
Demolish and rebuildRemoves the problemCompare with repair options by life-cycle cost (Chapter 3.8, Section 3.8.40).

Andrade et al. (2009) note that the efficiency of electrochemical treatments has traditionally been checked by switching off the protection current or by coring after treatment, and propose nondestructive checks (impedance, corrosion rate and potential, and the charge passed adjusted for concrete resistance). Ask for a measurable acceptance criterion in any electrochemical treatment contract.

7.4.8.4 Culverts: rehabilitate or replace

Da Silva and Goyns (2009) assessed two deep concrete sewers under a busy street that had deteriorated in different ways: one, made with dolomitic aggregate and a sacrificial layer, had lost material evenly; the other, cast in place with siliceous aggregate, had lost cement paste and exposed its aggregate. Because open-cut replacement was ruled out, both were rehabilitated by trenchless lining with a close-fitting continuous liner, and the annular space between liner and host pipe was grouted to prevent water paths. The same reasoning applies to deep culverts under track: open-cut replacement needs a track outage and a temporary shoofly or bridge, so lining, with the annulus grouted and any voids around the pipe filled, is often the preferred choice where the remaining pipe and surrounding soil can carry the load. Check the lined culvert’s hydraulic capacity with the reduced diameter (Chapter 3.5, Section 3.5.10).

7.4.8.5 Retrofitting a slope failure with a structure

After a rainfall-triggered failure of a road cut on a mountain pass, Kruger et al. (2009) compared three repairs: an anchored pile wall with a cantilevered deck, a mechanically stabilized earth wall, and a half-width viaduct on piers. Steeply dipping, weathered and jointed rock made isolated pier footings vulnerable to block and wedge failure, and the MSE wall could have been undercut by future slides, so the anchored pile solution was chosen: eight 4-ft-diameter bored piles at about 26-ft centers, about 46 ft long and socketed about 13 ft into competent rock, carrying a 200-ft-long cantilevered deck balanced by a buried slab, with re-stressable rock anchors and the slab bolted down to rock. A temporary soil-nail wall kept traffic moving during construction.

For railroad work: the same logic applies to a sidehill grade that has lost its outer shoulder: where the rock structure dips out of the slope, prefer continuous anchored piles socketed into rock over isolated footings or a reinforced fill that could be undercut (Chapter 7.1, Section 7.1.4; Chapter 6.3). Use re-stressable anchors so that load can be checked and restored during the structure’s life.

7.4.8.6 Fitting concrete condition into the asset program

  • Add concrete condition (cracking, spalling, corrosion staining, AAR, wall loss, leaking joints) to the condition examination of culverts, walls and abutments (Section 7.4.2), and record it as a defect rating (Chapter 3.8).
  • Treat deterioration mechanisms as preparatory factors in the trigger analysis (Chapter 3.8): a corroding culvert is a slow loss of margin until a storm or a train load finishes it.
  • Plan intervention early: by the rule of fives, protecting sound concrete or patching early is far cheaper than rebuilding a failed structure under traffic.

7.4.8.7 Sources

Papers in Alexander, M. G., Beushausen, H.-D., Dehn, F. and Moyo, P. (eds.) (2009). Concrete Repair, Rehabilitation and Retrofitting II. Proceedings of the 2nd International Conference on Concrete Repair, Rehabilitation and Retrofitting (ICCRRR), Cape Town, 2008. London: CRC Press/Balkema. Summaries are paraphrased and values converted to English units.

  1. Walraven, J. C. (2009). “Design for service life: How should it be implemented in future codes.” ICCRRR 2008, 3–10.Find source ↗
  2. Wiggenhauser, H. (2009). “Advanced NDT methods for the assessment of concrete structures.” ICCRRR 2008, 19–30.Find source ↗
  3. Andrade, C., Martínez, I., Castellote, M. and García de Viedma, P. (2009). “Efficiency control of electrochemical repair techniques.” ICCRRR 2008, 31–38.Find source ↗
  4. Angst, U. and Vennesland, Ø. (2009). “Critical chloride content in reinforced concrete – State of the art.” ICCRRR 2008, 149–150.Find source ↗
  5. Fischboeck, E. K. and Harmuth, H. (2009). “An Austrian experience with identification and assessment of alkali-aggregate reaction in motorways.” ICCRRR 2008, 191–192.Find source ↗
  6. Da Silva, V. A. and Goyns, A. M. (2009). “The aging of concrete sewers: Replace or rehabilitate.” ICCRRR 2008, 281–282.Find source ↗
  7. Johansson, A., Janz, M., Silfwerbrand, J. and Trägårdh, J. (2009). “Protection of concrete with water repellant agents – What is required to achieve a sufficient penetration depth?” ICCRRR 2008, 287–288.Find source ↗
  8. Streicher, P. E., Hoppe, G. E., da Silva, V. A. and Kruger, E. J. (2009). “The application of electrochemical chloride extraction to reinforced concrete bridge members.” ICCRRR 2008, 303–304.Find source ↗
  9. Bänziger, H., Vogelsang, J. and Schulze, G. (2009). “The corrosion protection of embedded steel reinforcement in reinforced concrete structures using galvanic anodes.” ICCRRR 2008, 305–306.Find source ↗
  10. Glass, G. K., Roberts, A. C. and Davison, N. (2009). “Re-alkalisation technology applied to corrosion damaged concrete.” ICCRRR 2008, 307–308.Find source ↗
  11. Bissonnette, B., Nuta, A., Morency, M., Marchand, J. and Vaysburd, A. M. (2009). “Concrete repair and interfacial bond: Influence of surface preparation.” ICCRRR 2008, 345–346.Find source ↗
  12. Kruger, E. J., Newmark, A. A. and Smuts, M. (2009). “Mountain pass slope failure retrofitted with half viaduct bridge structure.” ICCRRR 2008, 395–396.Find source ↗
← Previous · 7.0 Design Chapter 7.3 — Pavement Subgrade Evaluation
Next · 8.0 Reporting → Chapter 8.1 — Exploration Versus Investigation